Manufacturing method of aluminum alloy Anode assembly with high strength and high conductivity in Henan Chalco, including the following steps:
Step 1: aluminum ingots for electrolysis or remelting with purity of 99.6%, magnesium ingots with purity of 99.9% and al-5ti-b alloy rods were selected as raw materials.
Step 2: heat and melt the aluminum ingots to 780 ~ 800℃ in the melting furnace or directly inject the electrolytic primary aluminum at a temperature of 780 ~ 800℃, add magnesium ingots accounting for 0.7-0.8% of the total weight of the raw materials, stir and melt the aluminum alloy liquid, and then add the coating agent after refining and degassing;
Step 3: to aluminum alloy liquid temperature control during 730 ~ 740 ℃, the liquid aluminum alloy imported pouring shaft, according to the casting speed with thread feeding machine add Φ 9.5 millimeters in diameter in chute ti Al - 5 - B alloy rod online grain refining process for aluminum alloy liquid;
The fourth step: according to the requirements of casting blank chamfering, milling, punching and other mechanical processing to get qualified Anode assembly.
machine add Φ 9.5 millimeters in diameter in chute ti Al - 5 - B alloy rod online grain refining process for aluminum alloy liquid;
The fourth step: according to the requirements of casting blank chamfering, milling, punching and other mechanical processing to get qualified Anode assembly.